Santoprene™ 203-40

Категория TPV, Thermoplastic Vulcanizate
Производитель ExxonMobil Chemical
Торговая марка Santoprene™
Порт Китай Шанхайский порт
Торговые условия FOB, CFR, CIF
Платежное средство L/C, T/T, Western Union
PDF stRngE_Santoprene-203-40.pdf
Контактная информация
EMAIL US sales@su-jiao.com

Служба поддержки клиентов Вичат
Описание материалов:
It is a hard, colorable, universal thermoplastic vulcanized elastomer (TPV) in the thermoplastic elastomer (TPE) series. This material has good physical properties and chemical resistance at the same time, and is suitable for a wide range of fields. This brand of Shanduping TPV is a shear rate dependent product that can be processed on conventional thermoplastic injection molding, extrusion molding, blow molding, thermoforming or vacuum forming equipment. This is a polyolefin-based material that can be recycled in the production process.
Главная Информация
Характеристики
  • Хорошая стабильность размеров
  • Изоляция
  • Перерабатываемые материалы
  • Хорошая электрическая производительность
  • Хорошая прочность на разрыв
  • Хорошая окраска
  • Озоновая защита
  • Хорошая химическая стойкость
  • Сопротивление усталости
Используется
  • Электрические компоненты
  • Диафрагма
  • Фитинги для труб
  • Подвижный шарнир
  • Детали бытовой техники
  • Детали под крышкой двигателя автомобиля
  • Применение в автомобильной области
  • Применение потребительских товаров
Рейтинг агентства
  • UL QMFZ2
  • UL QMFZ8
Соответствие RoHS
  • Соответствие RoHS
Номер файла UL
  • E80017
Внешний вид
  • Натуральный цвет
Формы
  • Частицы
Метод обработки
  • Выдувное формование
  • Многократное литье под давлением
  • Коэкструзионное формование
  • Экструзия
  • Экструзионное выдувное формование
  • Экструзионный лист
  • Термоформовка
  • Экструзионное формование профиля
  • Вакуумная формовка
  • Литье под давлением
  • Литье под давлением
ФизическийНоминальное значениеЕдиница измеренияМетод испытания
Удельный вес
    -- 0.948g/cm³ASTM D792
    -- 0.950g/cm³ISO 1183
Сопротивление моющим средствам f4UL 2157
Сопротивление моющим средствам f3UL 749
ТвердостьНоминальное значениеЕдиница измеренияМетод испытания
Твердость дюрометра (Shaw D, 15 seconds, 23°C, 2.00mm)41ISO 868
ЭластомерыНоминальное значениеЕдиница измеренияМетод испытания
Растяжимое напряжение- Поперечный поток (100% Strain, 23°C)9.00MPaASTM D412, ISO 37
Прочность на растяжение- Поперечный поток (Break, 23°C)20.7MPaASTM D412, ISO 37
Растяжимое удлинение- Поперечный поток (Break, 23°C)610%ASTM D412, ISO 37
Прочность на разрыв- Поперечный поток
    23°C 167.0kN/mASTM D624
    23°C 267kN/mISO 34-1
Комплект сжатия
    70°C, 22 hr 354%ASTM D395B
    125°C, 70 hr 461%ASTM D395B
    70°C, 22 hr 554%ISO 815
    125°C, 70 hr 661%ISO 815
СтарениеНоминальное значениеЕдиница измеренияМетод испытания
Изменение прочности на растяжение в воздухе (150°C, 168 hr)-11%ASTM D573, ISO 188
Изменение максимального удлинения в воздухе (150°C, 168 hr)-15%ASTM D573, ISO 188
Изменение твердости дюрометра в воздухе (support d, 150°C, 168 hr)4.0ASTM D573, ISO 188
Изменение прочности на растяжение ASTM D471, ISO 1817
    23°C, 168 hr, in 10% hydrochloric acid 6.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 15% sodium chloride 4.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 2.5% detergent (Tide) 0.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 50% sodium hydroxide 4.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 95% ethanol -3.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 98% sulfuric acid -22%ASTM D471, ISO 1817
    23°C, 168 hr, in acetic acid 0.0%ASTM D471, ISO 1817
    23°C, 168 hr, in cyclohexane -2.0%ASTM D471, ISO 1817
    23°C, 168 hr, in methyl ethyl ketone 3.0%ASTM D471, ISO 1817
    23°C, 168 hr, in isopropanol 5.0%ASTM D471, ISO 1817
    23°C, 168 hr, in trichloroethylene 8.0%ASTM D471, ISO 1817
    100°C, 168 hr, in IRM 903 oil -26%ASTM D471, ISO 1817
    100°C, 168 hr, in deionized water 3.0%ASTM D471, ISO 1817
    125°C, 70 hr, in IRM 903 oil -27%ASTM D471, ISO 1817
    125°C, 168 hr, in IRM 903 oil -30%ASTM D471, ISO 1817
Изменение максимального удлинения ASTM D471, ISO 1817
    23°C, 168 hr, in 10% hydrochloric acid 5.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 15% sodium chloride 2.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 2.5% detergent (Tide) 0.0 0.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 50% sodium hydroxide 3.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 95% ethanol -2.0%ASTM D471, ISO 1817
    23°C, 168 hr, in 98% sulfuric acid -23%ASTM D471, ISO 1817
    23°C, 168 hr, in cyclohexane 2.0%ASTM D471, ISO 1817
    23°C, 168 hr, in methyl ethyl ketone 2.0%ASTM D471, ISO 1817
    23°C, 168 hr, in isopropanol 5.0%ASTM D471, ISO 1817
    23°C, 168 hr, in trichloroethylene 2.0%ASTM D471, ISO 1817
    100°C, 168 hr, in IRM 903 oil -28%ASTM D471, ISO 1817
    100°C, 168 hr, in deionized water 0.0%ASTM D471, ISO 1817
    125°C, 70 hr, in IRM 903 oil -33%ASTM D471, ISO 1817
    125°C, 168 hr, in IRM 903 oil -39%ASTM D471, ISO 1817
Изменение твердости дюрометра
    Support A, 23°C, 168 hr, in 10% hydrochloric acid -1.0ASTM D471
    Support A, 23°C, 168 hr, in 15% sodium chloride 2.0ASTM D471
    Support A, 23°C, 168 hr, in 2.5% detergent (Tide) 0.0ASTM D471
    Support A, 23°C, 168 hr, in 50% sodium hydroxide 1.0ASTM D471
    Support A, 23°C, 168 hr, in 95% ethanol 0.0ASTM D471
    Support A, 23°C, 168 hr, in 98% sulfuric acid 2.0ASTM D471
    Support A, 23°C, 168 hr, in acetic acid -1.0ASTM D471, ISO 1817
    Support A, 23°C, 168 hr, in cyclohexane -13ASTM D471, ISO 1817
    Support A, 23°C, 168 hr, in methyl ethyl ketone 0.0ASTM D471, ISO 1817
    Support A, 23°C, 168 hr, in isopropyl alcohol 2.0ASTM D471, ISO 1817
    Support A, 23°C, 168 hr, in trichloroethylene 1.0ASTM D471, ISO 1817
    Support A, 100°C, 168 hr, in IRM 903 oil -13ASTM D471
    Support A, 100°C, 168 hr, in deionized water 0.0ASTM D471, ISO 1817
    Support A, 125°C, 168 hr, in IRM 903 oil -15ASTM D471
    Support A, 23°C, 168 hr, in 10% hydrochloric acid -1.0ISO 1817
    Support A, 23°C, 168 hr, in 15% sodium chloride 2.0ISO 1817
    Support A, 23°C, 168 hr, in 2.5% detergent (Tide) 0.0ISO 1817
    Support A, 23°C, 168 hr, in 50% sodium hydroxide 1.0ISO 1817
    Support A, 23°C, 168 hr, in 95% ethanol 0.0ISO 1817
    Support A, 23°C, 168 hr, in 98% sulfuric acid 2.0ISO 1817
    Support A, 100°C, 168 hr, in IRM 903 oil -13ISO 1817
    Support A, 125°C, 168 hr, in IRM 903 oil -15ISO 1817
Изменение массы ASTM D471
    23°C, 168 hr, in 10% hydrochloric acid 0.10%ASTM D471
    23°C, 168 hr, in 15% sodium chloride 0.10%ASTM D471
    23°C, 168 hr, in 50% sodium hydroxide 0.0%ASTM D471
    23°C, 168 hr, in 95% ethanol -0.60%ASTM D471
    23°C, 168 hr, in 98% sulfuric acid 1.1%ASTM D471
    23°C, 168 hr, in acetic acid 1.2%ASTM D471
    23°C, 168 hr, in cyclohexane -3.4%ASTM D471
    23°C, 168 hr, in methyl ethyl ketone -12%ASTM D471
    23°C, 168 hr, in isopropanol -5.0%ASTM D471
    23°C, 168 hr, in trichloroethylene -1.0%ASTM D471
    100°C, 168 hr, in IRM 903 oil 35%ASTM D471
    100°C, 168 hr, in deionized water 1.4%ASTM D471
    125°C, 168 hr, in IRM 903 oil 44%ASTM D471
Изменение массы ISO 1817
    23.0°C, 168 hr, in methyl ethyl ketone -12%ISO 1817
    23.0°C, 168 hr, in isopropanol -5.0%ISO 1817
    23.0°C, 168 hr, in cyclohexane -3.4%ISO 1817
    23.0°C, 168 hr, in trichloroethylene -1.0%ISO 1817
    23.0°C, 168 hr, in 95% ethanol -0.60%ISO 1817
    23.0°C, 168 hr, in 50% sodium hydroxide 0.0%ISO 1817
    23.0°C, 168 hr, in 15% sodium chloride 0.10%ISO 1817
    23.0°C, 168 hr, in 10% hydrochloric acid 0.10%ISO 1817
    23.0°C, 168 hr, in 98% sulfuric acid 1.1%ISO 1817
    23.0°C, 168 hr, in acetic acid 1.2%ISO 1817
    100°C, 168 hr, in deionized water 1.4%ISO 1817
    100°C, 168 hr, in IRM 903 oil 35%ISO 1817
    125°C, 168 hr, in IRM 903 oil 44%ISO 1817
Изменение объема
    125°C, 70 hr, in IRM 903 oil 40%ASTM D471
    125°C, 70 hr, in IRM 903 oil 40%ISO 1817
ТепловойНоминальное значениеЕдиница измеренияМетод испытания
Температура ломкости -52.0°CASTM D746, ISO 812
RTI Elec 85.0°CUL 746
RTI Str 85.0°CUL 746
ЭлектрическийНоминальное значениеЕдиница измеренияМетод испытания
Диэлектрическая прочность (23°C, 2.00 mm)28kV/mmASTM D149
Диэлектрическая постоянная (23°C, 1.98 mm)2.30ASTM D150, IEC 60250
Сравнительный индекс отслеживания (CTI) PLC 0UL 746
Высокоусиленное дуговое зажигание (HAI) PLC 0UL 746
Высоковольтное сопротивление дуге к зажиганию (HVAR) PLC 5UL 746
Высоковольтная скорость отслеживания дуги (HVTR) PLC 1UL 746
Зажигание горячей проволоки (HWI) UL 746
    1.00 mm PLC 4UL 746
    1.50 mm PLC 3UL 746
    3.00 mm PLC 2UL 746
ВоспламеняемостьНоминальное значениеЕдиница измеренияМетод испытания
Огнестойкость UL 94
    1.00 mm HBUL 94
    1.50 mm HBUL 94
    3.00 mm HBUL 94
Дополнительная информация
如果适用,这是基于扇形浇口注塑成型的平板测试结果。拉伸强度、伸长率和拉伸应力沿垂直流动方向测定 - ISO 1 型,ASTM die C。25% 形变时的永久压缩变形。从埃克森美孚欧洲分支机构直接购买的所有产品都符合 REACH 法规。 对于埃克森 美孚未进口至欧洲的产品,用户应自行评估其是否满足 REACH 法规。
Юридическое заявление
未经埃克森美孚化工书面允许,这种产品包括其产品名称,不得在任何医疗应用领域予以使用或有关详细的产品监管信息,请联系客户服务。
ИнъекцияНоминальное значениеЕдиница измерения
Температура сушки 82.2°C
Время сушки 3.0hr
Рекомендуемая максимальная влажность 0.080%
Рекомендуемый Макс измельчения 20%
Задняя температура 193°C
Средняя температура 199°C
Передняя температура 204°C
Температура сопла 210 - 238°C
Температура обработки (расплава) 216 - 232°C
Температура формы 10.0 - 51.7°C
Скорость впрыска Fast
Back Pressure 0.345 - 0.689MPa
Screw Speed 100 - 200rpm
Тонаж зажима 4.1 - 6.9kN/cm²
Подушка 3.18 - 6.35mm
Отношение винта L/D 16.0:1.0 to 20.0:1.0
Коэффициент сжатия винта 2.0:1.0 to 2.5:1.0
Глубина вентиляционного отверстия 0.025mm
Инструкции по впрыску
Santoprene TPV与乙缩醛和PVC不相容。更多关于加工和模具设计的信息,请查阅我们的《注射成型指南》。
ЭкструзияНоминальное значениеЕдиница измерения
Температура сушки 82.2°C
Время сушки 3.0hr
Температура расплава 210°C
Температура матрицы 216°C
Back Pressure 5.00 - 20.0MPa
Инструкции по экструзии
Santoprene TPV与乙缩醛和PVC不相容。更多关于加工和模具设计的信息,请查阅我们的《挤出成型指南》。
Примечание
1 .C mould
2 .Method B, right-angle specimen (cut)
3 .Type 1
4 .Type 1
5 .Type a
6 .Type a
Тип материала Категория Производитель
TAROPRENE® 1 A25 M1N TPV Taro Plast S.p.A.
TAROPRENE® 1 A85 M1N TPV Taro Plast S.p.A.
Trexprene® D40BU TPV Mitsubishi Chemical Performance Polymers, Inc.
Unipren® Elastomers B3 PRTA010 55A UP314 TPV Petropol Industry and Trade of Polymers LTDA
Sarlink® TPV 4139D TPV Teknor Apex Company
Elastron® V V100.A73.B TPV Elastron USA, Inc.
Получите информацию об этом продукте следующим способом.
Телефон+086 13424755533
EMAIL US sales@su-jiao.com

Служба поддержки клиентов Вичат

Copyright © russianpolymer.com All Rights Reserved
Получите информацию об этом продукте следующим способом.

Служба поддержки клиентов Вичат
Свяжитесь с нами