Описание материалов:
Solid Makrolon® sheets are clear, polished, UV-stabilized polycarbonate sheets. They offer extreme impact strength that exceeds the physical properties of other products of their class. Makrolon® sheets resist temperatures of -100 to +120°C, exhibit high optical clarity and have a good fire rating.
Makrolon® GP clear 099 is a clear transparent sheet with high light transmission.
Makrolon® NR clear 099 is a transparent sheet with a matt finish and improved UV resistance on one side.
Makrolon® GP white 130 and white 150 are translucent sheets offering good light diffusion combined with a pleasant white color.
Makrolon® GP umbra 775 sheets are brown-colored and transparent.
Makrolon® FG clear 099 is a clear transparent sheet suitable for food-contact and medical applications.
Applications:
Typical applications for Makrolon® GP sheets include machine guards, lighting fixtures, signs, wall and door partitions. The sheets offer protection against involuntary breakage and wilfull destruction. Makrolon® GP sheets can be thermoformed, cold-curved and machined with ease.
| Главная Информация | |
|---|
| Добавка | |
| Характеристики | - Стабилизированный УФ
- Высокая ударопрочность
- Высокое разрешение
|
| Используется | |
| Внешний вид | - Белый
- Коричневый
- Прозрачный/прозрачный
|
| Формы | |
| Метод обработки | - Машинная обработка
- Термоформовка
|
| Физический | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Плотность | 1.20 | g/cm³ | ISO 1183 |
| Поглощение воды | | | ISO 62 |
| Saturated, 23°C | 0.30 | % | ISO 62 |
| Equilibrium, 23°C, 50% RH | 0.12 | % | ISO 62 |
| Механические | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Модуль растяжения | 2350 | MPa | ISO 527-2/1 |
| Tensile Stress (Yield) | > 60.0 | MPa | ISO 527-2/50 |
| Растяжимое напряжение (Yield) | 6.0 | % | ISO 527-2/50 |
| Номинальное растяжение при разрыве | > 50 | % | ISO 527-2/50 |
| Флекторный модуль 1 | 2350 | MPa | ISO 178 |
| Флекторный стресс 2 | 90.0 | MPa | ISO 178 |
| Воздействие | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Ударная прочность 3(23°C, Partial Break) | 80 | kJ/m² | ISO 179/1eA |
| Charpy Unnotched Impact Strength (23°C) | No Break | | ISO 179/1eU |
| Зубчатый изод Impact 4(23°C, Partial Break) | 90 | kJ/m² | ISO 180/A |
| Тепловой | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Heat Deflection Temperature | | | |
| 0.45 MPa, not annealed | 140 | °C | ISO 75-2/B |
| 1.8 MPa, not annealed | 128 | °C | ISO 75-2/A |
| Викат Температура размягчения | 148 | °C | ISO 306/B50 |
| CLTE-
Поток (23 to 55°C) | 6.5E-5 | cm/cm/°C | ISO 11359-2 |
| Теплопроводность (23°C) | 0.20 | W/m/K | ISO 8302 |
| Электрический | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Удельное сопротивление поверхности | 1.0E+16 | ohms | IEC 60093 |
| Сопротивление громкости | 1.0E+16 | ohms·cm | IEC 60093 |
| Диэлектрическая прочность (1.00 mm) | 34 | kV/mm | IEC 60243-1 |
| Относительная проницаемость | | | IEC 60250 |
| 100 Hz | 3.10 | | IEC 60250 |
| 1 MHz | 3.00 | | IEC 60250 |
| Коэффициент рассеивания | | | ASTM D150 |
| 100 Hz | 5.0E-4 | | ASTM D150 |
| 1 MHz | 9.5E-3 | | ASTM D150 |
| Воспламеняемость | Номинальное значение | Единица измерения | Метод испытания |
|---|
| Огнестойкость | | | UL 94 |
| > 1.5 mm, ALL | HB | | UL 94 |
| 0.8 to 1.4mm, ALL | V-2 | | UL 94 |
| > 10.0 mm, Clear 009 | V-0 | | UL 94 |
| Оптический | Номинальное значение | | Метод испытания |
|---|
| Индекс преломления 5 | 1.587 | | ISO 489 |
| Примечание |
|---|
| 1 . | 2.0 mm/min |
| 2 . | 2.0 mm/min |
| 3 . | 3 mm |
| 4 . | 3.2 mm |
| 5 . | Method A |